活化剂对活性炭处理矿山废水Mn2+的影响研究
|
周剑林,刘伟银,冯涛,曹运江,陈章,李志贤,陈国梁,陈远其
|
Effect of activators on adsorption ability of activated carbon to Mn2+ in mine wastewater
|
Jianlin Zhou,Weiyin Liu,Tao Feng,Yunjiang Cao,Zhang Chen,Zhixian Li,Guoliang Chen,Yuanqi Chen
|
|
表1 活性炭活化条件及其孔隙结构
|
|
|
样品 | 炭化温度/℃ | 炭化时间/min | 活化温度/℃ | 活化时间/min | 负载量/% | 比表面积/(m2·g-1) | 孔容/(cm3·g-1) | 亚甲蓝吸附量/(mg·g-1) | 碘离子吸附量/(mg·g-1) | SL-AC | 500 | 30 | 800 | 120 | — | 372 | 0.294 | 43.20 | 243.64 | H-AC | 500 | 30 | 800 | 120 | — | 330 | 0.261 | 56.77 | 239.92 | Na-AC | 600 | 30 | 900 | 240 | 5 | 438 | 0.315 | 85.34 | 328.33 | K-AC | 600 | 30 | 900 | 240 | 5 | 535 | 0.379 | 101.25 | 432.74 | Fe-AC | 600 | 30 | 900 | 240 | 5 | 275 | 0.208 | 45.92 | 181.46 |
|
|
|